Chinese Journal of Lasers, Volume. 52, Issue 12, 1202102(2025)

Effect of Heat Treatment on Microstructure of TiB2/Inconel718 Composites Fabricated by Laser Solid Forming

Huajing Zhai1, Fenggang Liu1、*, Fencheng Liu1, Qifan You1, Xiaobin Yu1, and Xuehao Gao2、**
Author Affiliations
  • 1School of Materials Science and Engineering, Nanchang Hangkong University, Nanchang 330063, Jiangxi , China
  • 2Ningbo Institute of Materials Technology and Engineering, Chinese Academy of Sciences, Ningbo 315000, Zhejiang , China
  • show less
    Figures & Tables(9)
    Tissue images of sample #1 fabricated by laser solid forming after HHT. (a) 1175 ℃; (b) 1200 ℃; (c) 1225 ℃; (d) 1250 ℃
    Tissue images of sample #2 fabricated by laser solid forming after HHT. (a) 1175 ℃; (b) 1200 ℃; (c) 1225 ℃; (d) 1250 ℃
    Tissue images of sample #3 fabricated by laser solid forming after HHT. (a) 1175 ℃; (b) 1200 ℃; (c) 1225 ℃; (d) 1250 ℃
    SEM images of laser solid formed TiB2/In718 composites after 1200 ℃ HHT. (a) Sample #1; (b) sample #2; (c)(d) sample #3
    Tissue morphologies of laser solid formed TiB2/In718 composites in DA heat treatment state. (a)(d)(g) Sample #1;
    Tissue morphologies of laser solid formed TiB2/In718 composites in STA heat treatment state. (a)(d)(g) Sample #1;
    • Table 1. Chemical compositions of Inconel718 alloy

      View table

      Table 1. Chemical compositions of Inconel718 alloy

      ElementCCrNiNbAlTi
      Mass fraction /%≤0.08017.000‒21.00050.000‒55.0004.750‒5.5000.300‒0.7000.750‒1.150
      ElementMoMnSiSPFe
      Mass fraction /%2.800‒3.300≤0.350≤0.350≤0.015≤0.015Bal.
    • Table 2. Heat treatment regime for laser solid forming of TiB2/In718 composites

      View table

      Table 2. Heat treatment regime for laser solid forming of TiB2/In718 composites

      Heat treatment processRegime
      HHT1175,1200,1225,1250 ℃
      DA720 ℃×8 h(AC)+620 ℃×8 h(AC)
      STA980 ℃×1 h(WC)+ 720 ℃×8 h(AC)+620 ℃×8 h(AC)
    • Table 3. Elemental analysis of precipitated phases (mass fraction, %)

      View table

      Table 3. Elemental analysis of precipitated phases (mass fraction, %)

      ElementNiBCrFeMoTiAlNb
      EDS16.4980.304.972.601.901.600.0903.20
      EDS21.6074.4010.801.605.401.200.0904.70
      EDS311.9077.602.902.700.151.600.0403.10
    Tools

    Get Citation

    Copy Citation Text

    Huajing Zhai, Fenggang Liu, Fencheng Liu, Qifan You, Xiaobin Yu, Xuehao Gao. Effect of Heat Treatment on Microstructure of TiB2/Inconel718 Composites Fabricated by Laser Solid Forming[J]. Chinese Journal of Lasers, 2025, 52(12): 1202102

    Download Citation

    EndNote(RIS)BibTexPlain Text
    Save article for my favorites
    Paper Information

    Category: Laser Forming Manufacturing

    Received: Dec. 3, 2024

    Accepted: Jan. 21, 2025

    Published Online: May. 22, 2025

    The Author Email: Fenggang Liu (printlfg@163.com), Xuehao Gao (gaoxuehao@nimte.ac.cn)

    DOI:10.3788/CJL241413

    CSTR:32183.14.CJL241413

    Topics