Journal of Inorganic Materials, Volume. 36, Issue 12, 1247(2021)

Tailoring MAX Phase Magnetic Property Based on M-site and A-site Double Solid Solution

Xiao ZHANG*, Youbing LI, Ke CHEN, Haoming DING, Lu CHEN, Mian LI, Rongrong SHI, Zhifang CHAI, and Qing HUANG
Figures & Tables(6)
Characterization results of (V, Nb)2(Sn, Fe)C after acid treatment
XRD patterns of (a) (V, Nb)2(Sn, Co)C, (c) (V, Nb)2(Sn, Ni)C, and (e) (V, Nb)2(Sn, Mn)C after acid treatment; SEM-EDS elemental mappings of (b) (V, Nb)2(Sn, Co)C, (d) (V, Nb)2(Sn, Ni)C, and (f) (V, Nb)2(Sn, Mn)C after acid treatment
Temperature dependent magnetization M-T curves for (a) V2(Sn, A)C and (b) V2(Sn, A)C (A = Fe, Co, Ni and Mn) at 0.1 T in the range of 2-100 K
Magnetic hysteresis loops of V2(Sn, A)C and V2(Sn, A)C (A=Fe, Co, Ni and Mn) at different temperatures in the range from -1 to 1 T, respectively
  • Table 1. Lattice parameters and atomic percentage of element in MAX phases

    View table
    View in Article

    Table 1. Lattice parameters and atomic percentage of element in MAX phases

    MAX phaseLattice parameterElement percentage/%Nb element in M site/% Magnetic element in A site/%
    a/nm c/nm c/aVNbSnA
    V2(Sn, Fe)C[23]0.29841.33454.471866.84-22.0511.11-33.50
    (V, Nb)2(Sn, Fe)C 0.30141.34474.462254.3213.3825.037.2719.7622.51
    V2(Sn, Co)C[23]0.29891.34094.486466.36-22.4411.19-33.28
    (V, Nb)2(Sn, Co)C 0.30161.34194.449356.4111.2324.607.7616.6023.98
    V2(Sn, Ni)C[23]0.29851.33574.475167.47-24.368.16-25.10
    (V, Nb)2(Sn, Ni)C 0.30211.34134.440256.8713.0021.668.4718.6128.10
    V2(Sn, Mn)C[23]0.29821.34034.494166.19-23.0710.74-31.76
    (V, Nb)2(Sn, Mn)C 0.30261.35094.464657.1010.8423.508.5615.9626.70
  • Table 2. Magnetic parameters of V2(Sn, A)C and (V, Nb)2(Sn, A)C (A = Fe, Co, Ni and Mn)

    View table
    View in Article

    Table 2. Magnetic parameters of V2(Sn, A)C and (V, Nb)2(Sn, A)C (A = Fe, Co, Ni and Mn)

    MAX phaseTC2 K20 K40 K
    HcMrMsHcMrMsHcMrMs
    V2(Sn, Fe)C 634580.591.733050.421.531520.181.08
    (V, Nb)2(Sn, Fe)C 632380.481.791740.371.67730.141.24
    V2(Sn, Co)C 663140.341.192240.261.051130.120.79
    (V, Nb)2(Sn, Co)C 533780.491.112400.331.001340.170.71
    V2(Sn, Ni)C 602760.301.541910.231.42940.101.12
    (V, Nb)2(Sn, Ni)C 531400.292.07960.191.83450.071.34
    V2(Sn, Mn)C 567800.260.985450.210.842060.070.63
    (V, Nb)2(Sn, Mn)C 571170.060.97750.040.90320.010.67
Tools

Get Citation

Copy Citation Text

Xiao ZHANG, Youbing LI, Ke CHEN, Haoming DING, Lu CHEN, Mian LI, Rongrong SHI, Zhifang CHAI, Qing HUANG. Tailoring MAX Phase Magnetic Property Based on M-site and A-site Double Solid Solution[J]. Journal of Inorganic Materials, 2021, 36(12): 1247

Download Citation

EndNote(RIS)BibTexPlain Text
Save article for my favorites
Paper Information

Category: EDITORIAL

Received: Mar. 3, 2021

Accepted: --

Published Online: Sep. 16, 2022

The Author Email: Xiao ZHANG (zhangxiao18@lzu.edu.cn)

DOI:10.15541/jim20210126

Topics