Journal of Inorganic Materials, Volume. 39, Issue 1, 51(2024)

Experimental Study on Low-velocity Impact and Residual Strength of SiC/SiC Composite Laminates

Jun WU1,2, Peifei XU1,2, Rui JING1,2, Dahai ZHANG1,2、*, and Qingguo FEI1,2
Author Affiliations
  • 11. School of Mechanical Engineering, Southeast University, Nanjing 211189, China
  • 22. Key Laboratory of Structure and Thermal Protection for High-Speed Aircraft, Ministry of Education, Nanjing 211189, China
  • show less
    Figures & Tables(16)
    Impact position and strain gauge position (a), and picture of the specimen of SiC/SiC laminate (b)
    Impact test machine and specimen fixture
    Size of CAI specimens (a) and TAI reinforcement piece (b)
    Pictures of post-impact compression test system (a) and post-impact tensile test system (b)
    Front (a-e) and back (f-j) damage morphologies of the specimens after being impacted with different energies
    CT images of the specimens with impact energy of 3 (A) and 5 J (B) along the thickness direction
    CT images of the specimens with impact energy of 3(A) and 5 J(B) along the width direction
    Position diagram of CT images of the specimen along width direction
    Impact responses of SiC/SiC specimen under different impact energy
    Strain-time curves of specimen during the impact process
    Impact damage behaviors of SiC/SiC laminates
    Moment of compression fracture of specimen under 3 J impact energy
    Tensile failure morphologies of specimens under different impact energies
    • Table 1. Impact test arrangement and residual strength test after impact

      View table
      View in Article

      Table 1. Impact test arrangement and residual strength test after impact

      Impact energy/JNumber of specimenResidual strength
      03TAI
      3CAI
      35TAI
      5CAI
      1, 2, 4, 5, 10, 202TAI
      2CAI
    • Table 2. CAI strength of undamaged and BVID specimens

      View table
      View in Article

      Table 2. CAI strength of undamaged and BVID specimens

      SpecimenImpact energy/JFmax/kN CAI strength/MPa
      C-0J-1042.18210.9
      C-0J-2037.38186.9
      C-0J-3040.66203.3
      C-3J-1335.13175.7
      C-3J-2334.88174.4
      C-3J-3332.28166.6
      C-3J-4328.34141.7
      C-3J-5331.22156.1
    • Table 3. TAI strength of undamaged and BVID specimens

      View table
      View in Article

      Table 3. TAI strength of undamaged and BVID specimens

      SpecimenImpact energy/JFmax/kN TAI strength/MPa
      T-0J-1058.77146.9
      T-0J-2065.94164.5
      T-0J-3071.79179.5
      T-3J-1343.62109.1
      T-3J-2345.16112.9
      T-3J-3343.72109.3
      T-3J-4345.48113.7
      T-3J-5345.01112.5
    Tools

    Get Citation

    Copy Citation Text

    Jun WU, Peifei XU, Rui JING, Dahai ZHANG, Qingguo FEI. Experimental Study on Low-velocity Impact and Residual Strength of SiC/SiC Composite Laminates[J]. Journal of Inorganic Materials, 2024, 39(1): 51

    Download Citation

    EndNote(RIS)BibTexPlain Text
    Save article for my favorites
    Paper Information

    Category:

    Received: Jun. 29, 2023

    Accepted: --

    Published Online: Mar. 28, 2024

    The Author Email: ZHANG Dahai (dzhang@seu.edu.cn)