Chinese Journal of Lasers, Volume. 45, Issue 6, 0602003(2018)

Microstructures and Properties of Joints in Ultra-Narrow-Gap Laser Wire Welding of P92 Steel and Inconel 625 Alloy Thick Plates

Hongyu Zhu, Pulin Nie*, Zhuguo Li, and Jian Huang
Author Affiliations
  • Shanghai Key Laboratory of Materials Laser Processing and Modification, School of Materials Science and Engineering,Shanghai Jiao Tong University, Shanghai 200240, China
  • show less
    Figures & Tables(17)
    Schematic of laser welding. (a) Groove; (b) welding
    Schematic of tensile and stress-rupture of samples at high temperature
    Macromorphology of welded joint
    Microstructures. (a) Weld zone; (b)(c) local magnifications of Fig.4(a)
    White particles in interdendritic zone
    Microstructure of HAZ of P92 steel
    HAZ of P92 steel. (a) CGHAZ; (b) FGHAZ
    Micro-hardness distributions of welded joints
    TEM images of martensite lath in CGHAZ of P92 steel. (a) Before heat-treatment; (b) after heat-treatment
    Tensile test results of welded joints. (a) Fracture position; (b) mechanical properties
    Microstructure of impact fracture. (a) Inconel 625 alloy; (b) welds; (c) P92 steel
    Tensile test of welded joints at high temperature
    Results of stress-rupture test at high temperature
    • Table 1. Chemical compositions of P92 steel and Inconel 625 alloy (mass fraction,%)

      View table

      Table 1. Chemical compositions of P92 steel and Inconel 625 alloy (mass fraction,%)

      ElementCNiFeCrMoWSiMnVNbTaTi
      P92 steel0.100.385Bal.9.010.571.720.370.550.250.070.31-
      Inconel 625 alloy0.02Bal.4.6022.109.20-0.090.05-3.45-0.18
    • Table 2. Process parameters of welding

      View table

      Table 2. Process parameters of welding

      Layer No.Laser power /kWWelding speed /(m·min-1)Defocusing /mmWire feeding rate /(m·min-1)
      14.01.200-
      2-123.3-3.50.42201.1
    • Table 3. EDS analysis results of white particles (mass fraction, %)

      View table

      Table 3. EDS analysis results of white particles (mass fraction, %)

      ElementTiVNbFeNiCrMoMn
      Value2.360.3340.959.0913.178.7211.300.21
    • Table 4. Impact test results of welded joints

      View table

      Table 4. Impact test results of welded joints

      MaterialInconel 625WeldP92
      Impact energy /J104.7887.8448.91
    Tools

    Get Citation

    Copy Citation Text

    Hongyu Zhu, Pulin Nie, Zhuguo Li, Jian Huang. Microstructures and Properties of Joints in Ultra-Narrow-Gap Laser Wire Welding of P92 Steel and Inconel 625 Alloy Thick Plates[J]. Chinese Journal of Lasers, 2018, 45(6): 0602003

    Download Citation

    EndNote(RIS)BibTexPlain Text
    Save article for my favorites
    Paper Information

    Category: laser manufacturing

    Received: Nov. 28, 2017

    Accepted: --

    Published Online: Jul. 5, 2018

    The Author Email: Nie Pulin (nplhxy@sjtu.edu.cn)

    DOI:10.3788/CJL201845.0602003

    Topics