Since the fabrication of the first superconducting nanowire single-photon detector (SNSPD) by Gol’tsman
Photonics Research, Volume. 9, Issue 3, 389(2021)
Saturation efficiency for detecting 1550 nm photons with a 2 × 2 array of Mo0.8Si0.2 nanowires at 2.2 K
Amorphous materials are attractive candidates for fabricating the superconducting nanowire single-photon detectors (SNSPDs) due to their superior tolerance and scalability over crystalline niobium nitride. However, the reduced superconducting transition temperature degenerates both operating temperature and saturation efficiency. Herein, the SNSPD (6.5 nm thickness and 50 nm width) based on the amorphous
1. INTRODUCTION
Since the fabrication of the first superconducting nanowire single-photon detector (SNSPD) by Gol’tsman
High internal detection efficiency (IDE) and operating temperature have always been the permanent pursuit for SNSPD; however, it is difficult to optimize the two features simultaneously [12]. The restriction stems from the internal mechanism of single photon detection by the superconducting materials. At the same time, it remains challenging for widely used NbN materials to fabricate such devices due to the crystal defects and large energy gap [13]. For this, researchers have developed novel superconductors based on amorphous materials, which have been demonstrated as promising candidates for SNSPDs [14,15]. Compared to the polycrystalline materials, the amorphous films show clear advantages in terms of tolerance and scalability. The nanowires fabricated by using amorphous materials appear to suffer from fewer constrictions, along with the high yield on the Si wafers [16]. The disordered structure offers a high degree of homogeneity and significant compatibility in the optical cavity. Moreover, the films with low energy gap are noted to be sensitive to midinfrared wavelengths [17]. Therefore, SNSPDs based on amorphous films have the potential to emerge as the desirable choice to detect the wavelengths from near-infrared to midinfrared.
According to the Bardeen–Cooper–Schrieffer relation [18], low energy gap results from low Tc, and vice versa. Based on this, the single-photon detectors fabricated from amorphous superconductors generally operate at low temperatures. For instance, the highest system detection efficiency (SDE) of 93% was achieved for the SNSPDs fabricated from amorphous WSi operated at 0.12 K at the National Institute of Standards and Technology (NIST) in 2013 [2], indicating that WSi-SNSPDs need to run below 1 K to achieve the optimal performance. In contrast, though the superconducting energy gaps of the MoSi thin films are comparable to that of WSi, their value is higher than 4 K [15]. Thus, the MoSi film becomes as a promising amorphous material for SNSPDs, which can be operated at temperature.
Sign up for Photonics Research TOC Get the latest issue of Advanced Photonics delivered right to you!Sign up now
Recently, MoSi-SNSPDs have presented an excellent performance, with a detection efficiency higher than 95% at 0.7 K [19]. Besides, it has been demonstrated that a 1 μm-wide MoSi superconducting strip is capable of single-photon detection. A large active area () of the microwire single-photon detector was fabricated, which exhibited the saturated photon counts at 0.3 K [16], suggesting that the MoSi film was competent for the fabrication of SNSPD with high efficiency and large area fabrication. As mentioned above, the single-photon detectors fabricated from amorphous superconductors generally operate at low temperatures to achieve the optimal performance, which hinders their development from the fundamental research phase to the practical application.
In this study, we fabricated SNSPDs with high-performance for both high Tc and high optical absorption coefficient of films.
2. EXPERIMENT
Figure 1.(a)
A. Growth of
In this study, the 6.5 nm-thick film has been grown on the polished and thermally oxidized silicon wafer by employing the DC magnetron sputtering from an alloy target (4-in. diameter, 1 in. = 2.54 cm) with the stoichiometry of Mo:. Before the film deposition, the sample is cleaned with Ar ion milling with the beam currents of 300 mA for 10 s and subsequently delivered to the chamber, followed by vacuum-pumping to . The sputtering process is performed at room temperature with 33 SCCM (standard cubic centimeter per minute) Ar gas, 45° throttle valve and 2 mTorr (1 Torr = 133.322 Pa) chamber pressure. Generally, the alloy target is presputtered for 5 min to clean the surface and stabilize the deposition conditions. The thickness of the film depends on the deposition rate (0.9 nm/s) and time.
Considering the poor antioxidant ability of the MoSi film, 4 nm-thick grown on the film is carried out in-situ to prevent oxidation. The film is deposited by an RF magnetron sputtering with RF power of 400 W in a 1:4 Ar and at 20 mTorr chamber pressure. Based on our previous experimental study, the chemical composition and crystalline structure of have been analyzed by using an Auger electron energy spectrometer (AES) and X-ray diffractometer (XRD). The results indicate that the sample has a Nb/N ratio of 5:6, along with a hexagonal structure [20]. Further, the film shows semiconducting electronic properties, in which the resistance rises as the temperature decreases, reaching at 4.2 K [21]. Thus, it is safe to suggest that the capping layer has no adverse impact on the superconducting film at low temperature. Simultaneously, the presence of the Nb5N6 capping layer also protects the film from degradation during the follow-up fabrication.
Figure 2.(a) Comparison of the resistivity versus temperature curve of the 6.5 nm (red) and 100 nm (black) films. (b)
An overview of the prior work on the superconducting properties of the MoSi films has been presented in Table 1. The optimization of the film sputtering recipes to operate the devices at high temperatures has been presented. As expected, the obtained in this study is higher than the other films, allowing the detectors to operate at . Comparison of the Different Stoichiometric Ratios of the MoSi Films in Terms of Bulk Film Stoichiometry Bulk 7.50 – – – 7.20 – – – 7.70 4.70 2.90 0.55 7.60 5.25 4.77 0.77 7.80 5.57 5.85 0.85
Figure 3.(a) Complex refractive index of the
B. Fabrication of
Figure 4.Estimation of the total etching time for the
3. RESULTS AND DISCUSSION
Figure 5.SEM images of the
Figure 6.(a)
The photon counting measurement is carried out with continuous tunable laser at 1550 nm, and the input photon flux is attenuated by the two serial variable attenuators to a level of photons/s, calibrated with a highly precise light power meter (Thorlabs-PM100D). The SNSPDs are illuminated by using a single module fiber coupled with the input light into detector. Figure 6(b) exhibits the photon count rate (PCR) as a function of the bias current () at different operating temperatures. Notably, the device has a saturated count rate ranging from 75 mK to 2.2 K. The saturation of the PCR versus curves indicates that the detector quantum efficiency is also saturated [17]. The observed behavior suggests that the device reaches its 100% internal detection efficiency [28]. Figure 6(c) demonstrates the internal detection efficiency of the 50 nm-width SNSPD, which reveals a sigmoidal dependence on the normalized bias current, with saturation at 0.8, where the DCR value is below 1 cps. To extract the saturation level of the detector, the bias dependence of IDE is fitted with an empirical sigmoid function [29]. The red solid line in Fig. 6(c) represents the fitting curve, where the maximum IDE reaches 100%.
Notably, as a proof of the array detector, a 4-pixel array device with 90 nm-width, a period of 200 nm, and an active area of has explicitly been fabricated. Figure 6(d) shows the normalized photon counts as a function of the bias current for the 4-pixel device operating at 2.2 K (inset depicting the I-V curve of one of the pixels). The is noted to be 9.5 μA with the hysteresis current of 1 μA, which is higher than the waveguide-integrated nanowire of 3.3 μA reported by Häußler [11], resulting in a higher signal-to-noise ratio. As demonstrated in the previous literature studies [28], the with a nanowire width of 110 nm and an active area of exhibited saturated internal efficiency at 2.3 K. The nanowire geometric defects and constrictions are proportional to the length, and the length of the nanowires is also proportional to the active area for the same size (width and pitch) of the nanowires. Therefore, it is extremely challenging to achieve the saturated efficiency at high temperatures for large active areas. In this study, the 4-pixel array device with 90 nm-width nanowires and an active area of has explicitly been fabricated, exhibiting the saturated intrinsic detection efficiency at a temperature of 2.2 K.
The I-V curves of the 4 pixels are noted to be similar for the switching current ranging from 9.0 μA to 9.5 μA. We have calculated the depairing current of SNSPD according to the equations presented by Korneeva
4. CONCLUSION
In conclusion, this work demonstrates the amorphous film exhibiting a high optical absorption coefficient in the visible to midinfrared range. The SNSPD fabricated from the film with 6.5 nm-thickness and 50 nm-width demonstrates the saturated intrinsic detection efficiency with sub 1 Hz dark count rate at a temperature of 0.2 K. Particularly, a uniform 4-pixel SNSPD has been successfully developed, exhibiting a saturation plateau for the photon counts at a temperature of 2.2 K. As a whole, the SNSPD based on films exhibits excellent advantages in operation temperature, spectral sensitivity, and internal detection efficiency.
[19] D. V. Reddy, R. R. Nerem, A. E. Lita, S. W. Nam, R. P. Mirin, V. B. Verma. Exceeding 95% system efficiency within the telecom C-band in superconducting nanowire single photon detectors. CLEO: QELS Fundamental Science, FF1A.3(2019).
Get Citation
Copy Citation Text
Feiyan Li, Hang Han, Qi Chen, Biao Zhang, Han Bao, Yue Dai, Rui Ge, Shuya Guo, Guanglong He, Yue Fei, Shuchao Yang, Xiaohan Wang, Hao Wang, Xiaoqing Jia, Qingyuan Zhao, Labao Zhang, Lin Kang, Peiheng Wu, "Saturation efficiency for detecting 1550 nm photons with a 2 × 2 array of Mo0.8Si0.2 nanowires at 2.2 K," Photonics Res. 9, 389 (2021)
Category: Optical Devices
Received: Oct. 15, 2020
Accepted: Dec. 29, 2020
Published Online: Mar. 2, 2021
The Author Email: Labao Zhang (Lzhang@nju.edu.cn)